AMS 5512 vs. ASTM A240 Grade 347: A Side-by-Side Spec Comparison for Sheet, Strip, and Plate

ams 5512 vs astm a240 grade 347 comparison

A drawing, a purchase order, or a customer’s material callout names AMS 5512. Your stock list says ASTM A240 Type 347. The buyer wants to know whether the two documents describe the same thing, the process engineer wants to know whether the coil will form the same way, and the quality engineer wants to know whether the mill certificate will survive an audit. All three questions land on the same desk at once, and the answer is not a simple yes or no.

Both documents describe a columbium-stabilized 18Cr-10.5Ni austenitic stainless steel, UNS S34700, in flat-rolled form. They are not, however, written for the same purpose or the same approval chain. AMS 5512 is an aerospace material specification issued by SAE International. ASTM A240/A240M is a general and pressure-vessel specification for chromium and chromium-nickel stainless plate, sheet, strip and 347 foil. One is built around aerospace quality assurance and identification; the other is built around pressure-vessel and general fabrication practice, with its dimensional and general rules delegated to A480/A480M.

This comparison covers what each document actually says about form and thickness scope, chemistry limits, mechanical properties and condition, tolerances and finish, testing and certification, and substitution. It is based on the published specifications and on supplier data sheets, not on in-house testing at a mill or laboratory. Where a requirement lives in a referenced document rather than in the specification itself, that is flagged rather than smoothed over.

Key takeaways

  • The two specifications overlap substantially on chemistry and mechanical minimums, but they diverge on scope, dimensional rules, and the paperwork chain.
  • A mill certificate that names one specification does not automatically satisfy the other, even when the heat would pass both chemistry tables.
  • Substitution in either direction needs documented purchaser or engineering approval; chemistry overlap is not authorization.
  • The controlled revision cited on the drawing or PO governs, not the revision summarized here.

Quick comparison: where the two specifications stand

ItemAMS 5512 (SAE)ASTM A240/A240M
Issuing body and typeSAE International; aerospace material specificationASTM International; material specification for pressure vessels and general applications
Product formsSheet, strip, and plate over 0.002 in (0.051 mm) in thicknessPlate, sheet, and strip; sheet/strip/plate definitions and dimensional rules sit in A480/A480M
Alloy identity18Cr-10.5Ni-0.80Cb (347), composition similar to UNS S34700Type 347, UNS S34700, among a large multi-grade table
Chemistry sourceTable 1 of AMS 5512Table 1 of A240/A240M
Mechanical basisTable 2A tensile requirements; solution heat treated conditionTable 2 minimum tensile, yield, elongation, hardness
ConditionSolution heat treatedAnnealed/solution-treated condition per the ordered grade and A480/A480M heat treatment rules
Dimensional tolerancesAMS 2242A480/A480M (Annex A2 inch-pound, Annex A3 for A480M)
Surface finishAS4194 nomenclature; descaled or bright finish consistent with A480/A480M appearance when solution treatment is not done in a bright atmosphereA480/A480M finish codes (No. 1, 2B, 2D, BA, No. 4, and others)
Sampling and testingAMS 2371 sampling; A751 chemistry; A370 mechanical; E290 bend where applicableA370 tensile, hardness per Table 2, cold bend only where Table 2 requires it, heat analysis, grain size for austenitic H grades
Identification and reportingAMS 2807 identification; reports per the specification’s reports sectionA480/A480M material test report and certification requirements
Check-analysis limitsAMS 2248A480/A480M

The table compares scope and requirements, not a like-for-like winner. AMS 5512 is written for aerospace material control, where sampling plans, identification marking, and reporting are part of the product definition. A240 is written for pressure-vessel and general fabrication, where the material specification defines chemistry and mechanical properties and a companion general-requirements document defines dimensions, finish, and inspection defaults. A cell that says “A480/A480M” is not a gap in A240; it is where A240 deliberately puts that requirement.

Scope and product form: which document covers your thickness and width?

AMS 5512 covers a corrosion- and heat-resistant steel in the form of sheet, strip, and plate over 0.002 in (0.051 mm) in thickness, supplied solution heat treated. Its application language describes parts requiring both corrosion and heat resistance, especially parts welded during fabrication, and parts requiring oxidation resistance up to 1500 °F (816 °C) — useful at that temperature only when stresses are low. The specification also states that usage is not limited to those applications, so the application paragraph describes typical use rather than a restriction.

A240 covers chromium, chromium-nickel, and chromium-manganese-nickel stainless steel plate, sheet, and strip for pressure vessels and for general applications including architectural, building, construction, and aesthetic applications. It is a multi-grade specification; Type 347 is one entry in a long Table 1. The product-form definitions and the dimensional tolerances are not in A240 itself. A240 clause 3.1 sends definitions, general requirements for delivery, ordering information, process, special tests, heat treatment, dimensions and permissible variations, workmanship, finish and appearance, number of tests, specimen preparation, retreatment, inspection, rejection and rehearing, material test report, certification, and packaging to the current edition of A480/A480M.

That hand-off has a practical consequence for anyone ordering narrow or thin material. A 0.05 mm foil sits right at the AMS 5512 floor of 0.051 mm, and anything thinner falls outside that document’s stated form scope. On the A240 side, the thickness itself is not the obstacle, but the tolerance that applies to it comes from A480/A480M, and A480/A480M defines strip as cold-rolled material under 3/16 in (5.00 mm) in thickness and under 24 in (600 mm) in width, with sheet defined as under 3/16 in and 24 in or wider. A precision slitter supplying 8 mm wide by 0.2 mm thick coil is squarely in strip territory, and the tolerance table that governs camber, thickness, and width is the one in the general-requirements document.

Scope notes on units and on reading the callout

  • A240 is expressed in both inch-pound and SI units, but unless the order specifies the “M” designation (A240M), the material is furnished in inch-pound units. Mixing values from the two systems is not permitted by the specification and can produce a nonconformance.
  • AMS 5512 states dimensions and properties in inch-pound units as primary, with SI values as approximate equivalents for information.
  • When a drawing cites a specification, read the full callout: specification number, revision or year date, grade or UNS number, condition, form, dimensions, finish, and any supplementary requirements. A bare “347 per AMS” or “347 per A240” leaves the tolerance document and the test list undefined.

Chemical composition: how close are the two chemistry tables?

Element, wt %AMS 5512 Table 1A240 Table 1, UNS S34700
Carbon0.08 max0.08 max
Manganese2.00 max2.00 max
Silicon1.00 max0.75 max
Phosphorus0.040 max0.045 max
Sulfur0.030 max0.030 max
Chromium17.00–19.0017.0–19.0
Nickel9.00–12.009.0–13.0
Columbium (Cb, = Nb)10×C min, 1.10 max10×C min, 1.00 max
Molybdenum0.75 maxnot specified for S34700
Copper0.75 maxnot specified for S34700

The two tables are close, but four differences can decide whether a heat passes one document and fails the other:

  • Silicon. AMS 5512 allows up to 1.00%; A240 caps S34700 at 0.75%. A heat at 0.85% Si is acceptable to AMS and outside A240.
  • Nickel. AMS 5512 runs 9.00–12.00%; A240 runs 9.0–13.0%. The AMS upper limit is tighter, so a heat at 12.5% Ni meets A240 and misses AMS.
  • Columbium. Both express the minimum as 10×C, but AMS 5512 caps Cb at 1.10% while A240 caps it at 1.00%. A heat with 1.05% Cb and 0.05% C meets the AMS formula and cap but exceeds the A240 cap.
  • Molybdenum and copper. AMS 5512 sets 0.75% max for each; the A240 S34700 row leaves both unspecified. Residual Mo or Cu from scrap can therefore sit inside A240 and outside AMS.

Two terminology points prevent a lot of confusion. First, columbium (Cb) and niobium (Nb) are the same element; A240 Table 1 carries a footnote saying so explicitly, and a certificate may use either symbol or “Cb+Ta.” Second, 347 and 347H are different grades. 347H is UNS S34709, with a carbon range of 0.04–0.10% and its own columbium formula (8×C min, 1.00 max in the A240 table). A certificate for 347H is not a certificate for 347, and neither is automatically a certificate for AMS 5512.

Scope note on analysis disputes. A product or check analysis is adjudicated under different tolerance rules depending on the document. AMS 5512 invokes AMS 2248 for chemical check analysis limits; A240 invokes A480/A480M, which permits the purchaser to perform a product analysis to verify identity and sets its own rules on how requirements may be made more stringent but not less. If a chemistry result is disputed, the applicable tolerance document is part of the argument, not an afterthought.

Mechanical properties and condition: same alloy, different acceptance basis

PropertyAMS 5512A240 Table 2, S34700
ConditionSolution heat treatedAnnealed/solution-treated per grade and A480/A480M
Tensile strengthTable 2A of the cited revision; the AMS numeric minimum was not retrieved for this comparison, so it is not confirmed as matching the A240 figure opposite75 ksi / 515 MPa min
Yield strength (0.2% offset)Table 2A of the cited revision; see tensile row30 ksi / 205 MPa min
ElongationTable 2A of the cited revision; see tensile row40% min in 2 in. or 50 mm
HardnessNot the primary acceptance basis in the AMS table95 HRBW / 201 HBW max for sheet and strip
Cold bendE290 bend testing where applicableRequired only where Table 2 specifies it; not required for S34700

The mechanical minimums are close enough that a well-made heat will usually clear both. The surrounding requirements are where the acceptance basis diverges. AMS 5512 requires solution heat treatment as the supplied condition and ties sampling and testing to AMS 2371, with mechanical testing to A370 and bend testing to E290 where applicable. A240 requires a tensile test per heat/condition lot, hardness testing as listed in Table 2, cold bend only for grades where Table 2 calls for it, heat analysis with product analysis when specified, and grain size for austenitic H grades. A240’s sampling and specimen rules come from A480/A480M, which also waives the hardness requirement when the material is too thin for Rockwell superficial testing — a detail that matters for thin strip.

A few cautions belong here. Typical property data sheets, including elevated-temperature tensile curves published by mills and distributors, are informational. They are not acceptance criteria under either document unless the purchase order makes them so. And A480/A480M carries a note that solution-annealing temperatures above 1950 °F (1066 °C) can impair the resistance to intergranular corrosion after subsequent exposure to sensitizing conditions in stabilized grades including 347 and 347H. Where intergranular corrosion is a concern, the purchaser should specify the corrosion test of A480/A480M section 18.2, conducted on sensitized specimens, which invokes the practices of ASTM A262. That test is a purchaser-specified requirement, not an automatic one.

Tolerances, finish, and surface: where the documents hand off

Neither document fully contains its own dimensional rules, and that is the single most common source of order disputes.

AMS 5512 invokes AMS 2242 for tolerances on corrosion- and heat-resistant steel sheet, strip, and plate, and AS4194 for sheet and strip surface finish nomenclature. Its supply condition is cold rolled, solution heat treated, and — unless solution treatment is performed in an atmosphere yielding a bright finish — descaled to a surface appearance in accordance with A480/A480M.

A240 invokes A480/A480M for dimensions and permissible variations, workmanship, finish and appearance, marking, packaging, and inspection defaults. A480/A480M carries the finish definitions (No. 1 hot-rolled annealed and pickled, 2D cold-rolled annealed and pickled, 2B cold-rolled bright, bright annealed, No. 4 polished, and others), the sheet/strip/plate definitions, the camber tables, and the edge-condition rules for cold-rolled strip.

For a fabricator ordering narrow strip, the practical implication is direct: camber, edge condition, thickness tolerance, width tolerance, and burr are governed by whichever tolerance document the PO cites. A certificate that carries both specification numbers does not by itself prove that the coil meets both sets of dimensional requirements. Under the dual-certification practice described by the British Stainless Steel Association, the product is expected to comply fully with the primary standard, while secondary standards may cover only cast chemistry and mechanical properties — dimensional tolerances are exactly the kind of requirement that may not be met for the secondary document.

What to put on the PO

  • Product form: strip, sheet, or plate, stated explicitly.
  • Dimensions: thickness × width × length, or coil with specified inside diameter and weight range.
  • Grade and UNS number, plus condition (solution heat treated, annealed and pickled, bright annealed).
  • Finish designation and whether one or both sides are polished.
  • Edge condition for strip (slit, rolled, deburred) and any burr limit.
  • The tolerance document: AMS 2242 or A480/A480M, cited by number.
  • Supplementary tests: IGC per A262 practice, grain size, impact, PMI, or others as required.
  • Certificate type and content, including whether EN 10204 3.1 is required.

Testing, inspection, and certification: what the paperwork must show

RequirementAMS 5512 expectsA240 expects
Specification designation and revisionSpecification number and revision letter on quotations, acknowledgments, and reportsProduct specification designation and year date on the material test report
Heat number and traceabilityIdentification per AMS 2807Marking and traceability per A480/A480M
Chemistry resultsAnalysis per A751; check analysis limits per AMS 2248Heat analysis; product analysis when specified; A480/A480M rules
Mechanical resultsTensile per A370, sampling per AMS 2371, bend per E290 where applicableTensile per A370, one per heat/condition lot; hardness per Table 2
Heat treatment conditionSolution heat treatedAnnealed/solution treated per grade and A480/A480M
Grain sizeNot a routine requirement of the base specificationRequired for austenitic H grades per E112
FinishDescaled or bright, consistent with A480/A480M appearanceFinish code per A480/A480M
Supplementary testsAs specified by purchaserAs specified by purchaser (for example A262 IGC, Charpy impact per Supplementary Requirement S1, 1% offset yield per S3)
CertificationReports per the specification’s reports section; unauthorized exceptions prohibitedMaterial test report and certification per A480/A480M

For AMS 5512, the testing chain runs through AMS 2371 for quality assurance sampling and testing, ASTM A751 for chemical analysis, ASTM A370 for mechanical testing, and ASTM E290 for bend testing where applicable. Identification follows AMS 2807. The revision history matters at incoming inspection: AMS 5512 Rev. M, revised November 2018, revised the chemical analysis standard, adjusted the number of significant digits for tensile strength in Table 2A, prohibited unauthorized exceptions, and revised the reports and identification clauses. A certificate citing an earlier revision may not reflect those changes, which is one reason the revision letter belongs on the purchase order.

For A240, the required tests are tensile, hardness, cold bend only where Table 2 requires it, heat analysis with product analysis when specified, and grain size for austenitic H grades. The material test report must reference the product specification designation and year date indicating that the material was manufactured, sampled, tested, and inspected in accordance with the product specification. A480/A480M also permits the manufacturer to indicate more than one type of steel on a single report when certifying to more than one type, which is the mechanism behind multi-grade certificates.

One clarification that saves arguments at incoming inspection: EN 10204 3.1 is a certificate type, not a material specification. It describes the kind of inspection document issued with the goods; it does not substitute for naming AMS 5512 or A240 on the order, and it does not by itself establish which specification’s requirements were tested.

Can one substitute for the other? Dual certification and approval

Because both documents describe UNS S34700 flat-rolled product, a single heat can often be produced to meet both chemistry and mechanical tables. That is why dual- or multi-certified supply exists, and why a stockholder can hold one coil and sell it against several callouts.

The boundary needs to be drawn clearly. Dual certification is a commercial practice, not something either standards body recognizes. The BSSA guidance is explicit that multi-certified products should not be assumed to fully comply with all requirements of each standard mentioned, taken individually — dimensional tolerances are the standard example — and that the product should comply with all requirements of the primary standard, with secondary standards typically covering cast chemistry and mechanical properties only. There are no universally agreed rules for secondary conformance, so the scope of a multi-certificate should be confirmed with the mill that issued it.

For aerospace or defense flow-down, substituting A240 material for an AMS 5512 callout — or the reverse — requires purchaser or engineering approval documented on the PO or drawing. A mill certificate alone does not authorize it, and neither does a chemistry table that happens to overlap.

A short decision guide

  • Dual-certified stock makes sense for mixed-order stockholding, for general fabrication where no code stamp or aerospace flow-down applies, and where the buyer has confirmed in writing what the secondary certification covers.
  • Dual-certified stock is not enough for code-stamped pressure equipment, for aerospace or defense flow-down, or where the order specifies IGC testing, grain size, or dimensional tolerances that only one of the cited documents actually governs.
  • In every case, the substitution decision belongs on the PO or drawing, with the approving function named.

Practical resource: a spec cheat-sheet for the shop floor

A one-page comparison sheet earns its place on a desk if it carries the items that get checked repeatedly. A useful version contains:

  • The scope and thickness thresholds for each document, including the 0.002 in (0.051 mm) AMS floor and the A480/A480M sheet-versus-strip definitions.
  • The two chemistry columns side by side, with the Cb formula written out and the silicon, nickel, and Cb cap differences highlighted.
  • The mechanical minimums and the condition each document specifies.
  • The tolerance and finish references: AMS 2242 and AS4194 on one side, A480/A480M on the other.
  • The certification checklist from the previous section, condensed to the items an incoming inspector actually verifies.

If Seather Technology offers a downloadable spec cheat-sheet of this kind on its site, it may be a reasonable starting point for a shop-floor reference. Seather also supplies 347 stainless sheet, plate, strip, and coil alongside its fabrication services, so a buyer working through a 347 callout can ask for the material and, where offered, such a reference sheet. Two limits apply. The cheat-sheet is a convenience, not a controlled document, and it does not replace the governing specifications. The controlled revision cited on the PO always governs, and any conflict between a summary sheet and the specification resolves in favor of the specification.

Verdict: which specification applies to your order?

SituationGoverning document
Aerospace drawing citing AMS 5512AMS 5512, at the revision cited, with AMS 2242 tolerances and AMS 2371 sampling
ASME code pressure vessel citing SA-240ASME SA-240, which adopts A240 technical requirements, plus ASME documentation and inspection requirements
General fabrication citing A240A240/A240M plus A480/A480M for dimensions, finish, and general requirements
Mixed or dual-certified stockThe primary standard named first on the certificate, confirmed in writing for scope; substitution still needs approval

The core rule is short. The drawing, PO, or code citation decides which document governs. Chemistry overlap does not authorize substitution. The certificate must name the specification and revision it actually meets, and a multi-certificate should be read for what it covers, not for what its letterhead implies.

Before ordering, confirm four things: the revision in effect for the cited specification, any supplementary tests the application needs (IGC per A262, grain size, impact), the tolerance document that will govern dimensions and edge condition, and the certificate type and content the quality system requires.

Frequently asked questions

Is AMS 5512 the same as ASTM A240 347? They describe the same alloy family and the same UNS number, S34700, in flat-rolled form, but they are different documents with different issuing bodies, scopes, and approval chains. AMS 5512 is an aerospace material specification; A240 is a pressure-vessel and general-application specification that delegates dimensions and general requirements to A480/A480M.

Can A240 347 substitute for AMS 5512? Only with documented purchaser or engineering approval on the PO or drawing. Chemistry overlap is not authorization, and a mill certificate naming A240 does not by itself satisfy an AMS 5512 callout.

What is the difference between 347 and 347H? 347 is UNS S34700 with 0.08% max carbon; 347H is UNS S34709 with 0.04–0.10% carbon and its own columbium formula. They are distinct grades, and a certificate for one is not a certificate for the other.

Does a dual-certified certificate cover both specifications fully? Typically the primary standard is fully covered, while secondary standards cover cast chemistry and mechanical properties only. Dimensional and general requirements may not be met for the secondary document, so confirm the scope with the issuing mill.

What does “10×C min” mean for columbium? The columbium (niobium) minimum scales with the actual carbon content of the heat — ten times the carbon percentage — subject to an absolute maximum, which is 1.10% in AMS 5512 and 1.00% in A240 for S34700. A higher-carbon heat therefore requires more columbium to meet the same formula.

Which document covers tolerances? AMS 2242 for AMS 5512, and A480/A480M for A240. Neither material specification carries its own full dimensional tables.

Share:

Recent Posts

Superalloy Material Traceability: From Mill Heat to Finished Part

Introduction The expensive failure this guide addresses is not a cracked forging. It is a conforming forging whose paperwork cannot be tied back to the melt that produced it. The part may be dimensionally perfect, correctly heat treated and metallurgically sound, yet if the heat number on the mill certificate cannot be connected through conversion,

Machining Inconel 718: Material and Drawing Factors That Affect Cost

Inconel 718 is expensive to machine for a reason you can measure at the cutting edge. The alloy’s thermal conductivity is low — under 11.4 W/m·K according to one 2026 turning study — so heat generated by the cut does not leave with the chip. It accumulates in the tool. In dry turning, cutting temperatures

Talk to an Expert
Discuss Nickel Alloys, Stainless Steels, and Raw Materials and Custom Alloy Fabrication Components for Your Industrial Project
Scroll to Top

Request A Quote