Inconel 718 is an age-hardenable nickel alloy: it is solution treated at high temperature to dissolve the strengthening elements, then aged at lower temperature to precipitate the phases that give it strength. Which of those stages has already been performed when the material reaches your dock is decided by the heat-treatment line on your purchase order. The same alloy, from the same mill, ships solution treated only, solution treated and aged, or to one of several AMS conditions that fix the solution temperature and the aging cycle. The line you write determines what the supplier owes you, what you can cut, and which properties you can certify.
The failure this article addresses is not a bad heat of metal. It is material that is metallurgically sound and still wrong for your routing — aged bar that was supposed to be machined soft, or soft bar that was supposed to arrive with certified aged properties. The sequence below is written to be copied: decide the delivered condition, match it to your machining sequence, name it with its governing specification, write the line unambiguously, define the lot and coupon, and require the documents that prove what was done.
Decide the delivered condition before you write anything
Three delivery states cover most Inconel 718 orders, and the choice between them is really a question of who runs the final age.
Solution treated only. This is the default under ASTM B637, the standard specification for precipitation-hardening nickel alloy bars, forgings, and forging stock. Section 6.1 states that unless otherwise specified, material shall be supplied in the solution treated condition, suitable for subsequent age hardening. Section 6.2 then requires that the solution-treated material be capable of meeting the tensile, hardness and stress-rupture requirements after the precipitation hardening treatment in Table 2. In practice you receive soft, formable, machinable stock with a demonstrated capability — not with certified aged properties.
Solution treated plus aged. Under B637 §6.3, when material is supplied in the solution treated plus aged condition, the Table 3 and Table 4 requirements apply with the Table 2 precipitation treatment, or as agreed between purchaser and manufacturer as part of the purchase contract. Here the supplier runs the age and certifies the result.
An AMS condition that fixes the solution temperature. Aerospace and many energy drawings call out an AMS specification rather than B637. The three commonly encountered for 718 bar, forgings and rings are:
| Specification | Delivered condition | Solution treatment |
|---|---|---|
| AMS 5662 | Solution heat treated, precipitation hardenable | 1775 °F (968 °C), sub-solvus |
| AMS 5663 | Solution and precipitation heat treated | Sub-solvus, plus the two-step age |
| AMS 5664 | Solution heat treated, precipitation hardenable | 1950 °F (1066 °C), super-solvus |
A published comparison of the three specifications notes that AMS 5662 and 5663 both call out the same sub-solvus solution treatment — roughly 941 °C to 1010 °C for a time based on section thickness, followed by air cooling or faster — and that the difference between them is the inclusion of the aging treatment in 5663. AMS 5664 places the solution treatment above the delta-phase solvus and pairs it with a longer aging cycle. That is the practical content of the choice: 5662 and 5664 both deliver material you will age yourself, but they do not deliver the same starting microstructure, and 5663 delivers material already aged.
The default rule is easy to lose. B637 Table 2 carries a footnote stating that the purchaser shall designate on the purchase order or inquiry any partial stage of heat treatment required on material to be shipped. If you want the supplier to stop after solution treatment, or to perform only the first aging step, the order has to say so; silence is read against the default.
Before writing anything, settle three questions: who holds the furnace for the final age, who holds the risk if the aged properties miss, and whose name signs the property report. The answers point to the condition.
Match the condition to your machining sequence
For a part that will be rough-machined before final aging, ordering solution-treated stock and aging after rough machining is usually the sequence that lets you cut soft material and still finish with full properties. Ordering solution-treated-and-aged stock means you machine already-hardened material, and the supplier’s age is the one that counts.
The trade-offs are concrete. Aged stock gives you certified tensile, hardness and stress-rupture results at receiving, and it removes an operation and its pyrometry from your routing. It costs tool life — Inconel 718 in the aged condition is hard and strain-hardening, and a published comparison of machining conditions notes that annealed material provides easier machining and longer tool life, while aged material gives a slightly better finish. Solution-treated stock gives you machinability but pushes the aging operation, its furnace qualification, and its verification onto you or your heat treater.
The constraint that decides the sequence is thermal. Aging precipitates the strengthening phases from elements held in solution; the Special Metals technical bulletin describes the precipitation reaction as occurring in the range of 1100 °F to 1500 °F, and notes that for it to take place properly the aluminum, titanium and niobium must still be in solution. Any later exposure hot enough to re-dissolve or overage those phases changes the properties you certified. So the sequence — solution treat, rough machine, age, finish machine — has to be fixed before the PO is written, not discovered at the machine when someone asks whether the stock can take another thermal cycle.
One related point worth writing into the routing rather than the PO: heat treatment in air above roughly 1500 °F produces oxidation that ordinary finishing may not fully remove. A NASA heat-treat process specification for nickel and cobalt alloys requires a minimum of 0.010 in. removal during final machining after air heat treatment. If your final age is an air furnace operation on a near-net part, the machining allowance and the heat-treat sequence interact.
Name the condition and the specification together
A condition word alone is not a specification. “Aged,” “annealed,” “heat treated,” “stress relieved” each describe an intention, not a controlled cycle with defined temperatures, tolerances, test methods and acceptance criteria. A specification number alone is not sufficient either: AMS 5662 and AMS 5664 are both solution-treated, precipitation-hardenable conditions, and the number tells you which solution treatment was run, not whether an age was performed.
The discipline is to pair them on every line: alloy and UNS number (N07718), product form, the governing specification with its revision letter, and the condition as that specification defines it — including the solution temperature regime where an AMS variant fixes it.
The AMS 5662/5663/5664 distinction shows why the number matters. All three cover 718 bar, forgings and rings. AMS 5662 delivers 1775 °F solution-treated, precipitation-hardenable material. AMS 5663 delivers solution and precipitation heat treated material — the same sub-solvus solution treatment, plus the age. AMS 5664 delivers 1950 °F solution-treated, precipitation-hardenable material, a super-solvus start that is paired with a different, longer aging cycle when the material is aged. Same alloy, three different thermal histories, two different delivered states.
A caution about cross-references. Specification pages list each other freely — AMS 5664 cross-references AMS 5662 and 5663, and both cross-reference ASTM B637 — and a mill certificate may cite a cross-referenced designation. A cross-reference is a pointer, not a demonstration that the delivered condition satisfies the specification your drawing calls out. If the cert cites a different document than the one on the drawing, treat it as an open question to resolve before acceptance, not as equivalence.
Write the heat-treatment line so it cannot be misread
The heat-treatment line should be written so that a supplier reading it in isolation, without your drawing or your routing, cannot deliver something you will reject. Four patterns cover most orders.
Solution-treated-only stock, buyer ages in-house:
Alloy: Inconel 718, UNS N07718. Form: [bar / forging / plate], [dimensions]. Specification: ASTM B637, [revision]. Condition: solution treated only, suitable for subsequent age hardening, per B637 §6.1. Aging to be performed by purchaser. Certification and test report per B637 §15 required.
Solution-treated-and-aged stock, supplier certifies properties:
Alloy: Inconel 718, UNS N07718. Form: [bar / forging], [dimensions]. Specification: ASTM B637, [revision]. Condition: solution treated plus aged per B637 §6.3, precipitation hardening treatment per B637 Table 2. Tensile, hardness and stress-rupture properties to Table 3 and Table 4 to be certified from coupons aged with the production lot.
A specified AMS condition:
Alloy: Inconel 718, UNS N07718. Form: [bar / forgings / rings], [dimensions]. Specification: AMS 5663, [revision]. Condition: solution and precipitation heat treated as defined by AMS 5663. Supplier to perform all heat-treatment stages and certify properties to the specification. Heat-treat chart and pyrometry records required with shipment.
Material where the buyer will age in-house against an AMS solution treatment:
Alloy: Inconel 718, UNS N07718. Form: [bar], [dimensions]. Specification: AMS 5662, [revision]. Condition: solution heat treated, precipitation hardenable, as defined by AMS 5662. No aging to be performed by supplier. Purchaser will age after machining.
Now the failure modes. “Heat treated per spec” leaves the supplier to choose the stage. “Aged” names an outcome without a cycle, a test method or acceptance criteria. “Stress relieved” is not a condition defined for 718 delivery in these specifications and will be interpreted differently by different suppliers. “Per AMS 5663 or equivalent” is the most expensive of the four, because “or equivalent” invites a substitution you have no basis to audit — the supplier’s equivalent may be a different solution temperature, a different aging cycle, or a cross-referenced document. If you would not accept the substitute, do not write the escape clause.
Finally, do not transcribe the aging schedule onto the line. Refer to the specification’s table. A schedule copied onto a PO becomes a private, uncontrolled document the moment the published table is revised, and the copy will not carry the tolerances, the cooling rates, or the test methods that give the numbers meaning.
Define the lot and the test coupon in the order
Lot definition belongs on the purchase order because it determines how much testing you are buying and what a certificate actually covers. Under ASTM B637 §9.1.1, a lot for chemical analysis consists of one heat. Mechanical testing is then performed per lot: the B637 test schedule calls for one chemical analysis, one tension test, one hardness test and one stress-rupture test per lot.
What “one test per lot” commits the supplier to depends on the product form, because specimen location is defined by the form. For bar and rod, specimens come from the product; for forgings, the specification’s property tables carry footnotes for specimens machined tangentially from near the center of large disk forgings or radially from thick rings. If you are buying a large forging, the coupon location is part of what you are accepting, and it should be visible in the test report.
Practical PO language:
- State the lot definition you will accept, referencing the governing specification’s definition rather than inventing one.
- Require that test coupons be traceable to the lot and heat number.
- Require that coupons be aged with the production lot whenever properties are certified in the aged condition.
- Require that coupons be identified by lot certification number and work order.
The last two points are where receiving disputes concentrate. A coupon aged separately from the parts, in a different furnace or on a different cycle, produces a certificate that describes the coupon and not the shipment. If your order certifies aged properties, the coupon must see the same thermal cycle as the parts it represents. NASA’s nickel and cobalt heat-treat process specification makes the same point in the aerospace idiom: sample parts are to be machined from the same lot of raw stock and processed before heat treatment in an identical manner as the finished parts, and coupons are to be individually labeled with the material lot certification number and work order number.
Close the ambiguity explicitly. Write whether certified properties come from a coupon given the same thermal cycle as the parts, and require the supplier to state on the certification that this was done.
Require the documents that prove the condition
Documentation is not an afterthought to the heat-treatment line; it is part of it, because under B637 most of it is owed to you only if the order asks. Section 15 provides that when specified in the purchase order or contract, a producer’s or supplier’s certification shall be furnished that the material was manufactured, sampled, tested and inspected in accordance with the specification and found to meet the requirements — and, when specified, a report of the test results. Silence on the PO means silence at receiving.
Build the receiving package into the order:
| Document | What it proves | PO clause that obtains it |
|---|---|---|
| Mill or fabricator certification and test report | Chemistry, tensile, hardness, stress-rupture results per lot | “Certification and test report per B637 §15 required” |
| Heat-treat chart or furnace record | The cycle actually run, with times and temperatures | “Heat-treat chart for each lot required with shipment” |
| Pyrometry evidence | That the furnace and instruments were in calibration and the work zone was surveyed | “TUS and SAT records current at time of processing to be made available” |
| Traceability link | That the chart, lot and coupon belong together | “Chart to identify lot, heat number and work order” |
On pyrometry, keep the scope straight. AMS 2750 governs temperature measurement and control — how temperature is measured, recorded and verified — and does not define heat-treat process recipes. A compliance guide for the specification states the distinction plainly: the actual time-at-temperature recipes and material-specific requirements come from separate process specifications. So citing AMS 2750 on a PO tells the supplier what pyrometry discipline you expect behind the cycle; it does not tell them which condition to deliver. The condition still has to be named.
If the work is aerospace, the pyrometry callout usually includes a furnace class and instrumentation type, and those are set by the governing process specification rather than chosen for preference. A higher class is not automatically better; it carries a heavier calibration and survey burden that shows up in price. Confirm the required class with the heat treater before releasing the order rather than specifying the tightest available.
Catch the common receiving failures at the PO stage
Most receiving rejections on 718 trace to a clause that was never written. The mechanisms are worth knowing because each one points to a specific fix.
Wrong condition delivered. The supplier shipped solution-treated material against a drawing that assumed aged, or aged material against a routing that needed to machine soft stock. The certificate is internally consistent; the material is simply not what the routing assumed. The preventing clause is the condition line naming the stage and the party performing it.
Hardness outside the specified range. Hardness failures often trace to an ambiguous condition line — the supplier aged to a different cycle than the one your acceptance limit assumes — or to a coupon aged differently from the parts. B637 Table 3 sets a minimum Brinell hardness for 718 in the solution plus precipitation hardened condition; a result below it usually means the age was incomplete or the coupon did not see the production cycle. The preventing clauses are the named condition and the coupon-aged-with-lot requirement.
Missing or unmatched charts. The supplier never produced a chart because the PO never asked for one, or produced charts that cannot be tied to the shipment. The preventing clause is the documentation requirement, written as a condition of shipment rather than a request.
Lot or heat number mismatch between cert and parts. The lot was never defined on the order, so the supplier’s lot boundaries and yours differ. The preventing clause is the stated lot definition plus the requirement that product marking carry the condition and the specification number — B637 §16 requires each bundle or shipping container to be marked with the material name, condition (temper), specification number, size, weights, consignor and consignee, and contract or order number.
Properties certified from a non-representative coupon. The coupon was aged separately, or taken from a different location than the specification requires for the product form. The preventing clause is the coupon traceability and same-cycle requirement.
None of these require a statistic to be credible. Each is a mechanism with a clause that closes it.
Can you just put the aging temperature and time on the PO?
Usually not, and the recommendation is to reference the governing specification for the schedule and use the PO to state which stage is performed, who performs it, and what evidence is required.
The reason is that a transcribed schedule is a private specification. It has no controlled revision, so when the published table changes your PO does not. It has no defined test method, so the supplier can meet your numbers and still hand you a certificate you cannot compare to anything. It has no lot or coupon rules, so the properties may come from a specimen that never saw the production cycle. And it has no acceptance criteria beyond the numbers themselves — the supplier can hit your temperature and time and still deliver material that fails the specification’s tensile or stress-rupture requirements, because those requirements were never invoked.
There is a legitimate case for a buyer-specified non-standard cycle: a repair, a re-age after a weld, a part where the standard cycle has been shown unsuitable and a cycle has been agreed with the supplier and validated. B637 itself contemplates this — §6.3 allows the precipitation hardening treatment of Table 2 “or as agreed upon between the purchaser and the manufacturer as part of the purchase contract.” If you take that route, the order must carry the full cycle with tolerances and cooling rates, the acceptance properties, the test methods, and the coupon and lot rules. In other words, it must carry everything the published specification would have carried. A cycle written as two temperatures and two hold times does not.
Verify the order before it goes out
Run this against any Inconel 718 PO line before it goes out. It takes about five minutes and prevents the receiving hold.
- Alloy and UNS number stated: Inconel 718, UNS N07718.
- Product form and dimensions stated: bar, rod, forging, forging stock, plate, sheet — with size and quantity.
- Governing specification named with its revision letter: ASTM B637, AMS 5662, AMS 5663, AMS 5664, or the drawing’s own callout.
- Condition named as that specification defines it, including the solution temperature regime where an AMS variant fixes it.
- The stage or stages to be performed identified: solution only, solution plus age, or full heat treatment.
- The party performing each stage identified: supplier, purchaser, or a named heat treater.
- Lot definition stated, and coupon traceability and same-cycle aging required where aged properties are certified.
- Certification, test report, heat-treat chart and pyrometry records required as a condition of shipment.
- Inspection or witness rights stated if you want them — B637 §13 makes inspection a matter to be agreed in the purchase contract, and §4.1.10 requires the order to state which tests or inspections are to be witnessed.
- Product marking requirements stated, including condition and specification number per B637 §16.
If every box is checked, the line says what condition you are buying, who performs each stage, what the supplier must prove, and what you will accept at receiving. That is the whole of the exercise: the heat-treatment line is a specification decision, and the sequence above is how to make it deliberately rather than by default. Seather Technology’s fabrication scope covers nickel alloy processing from material analysis through heat treatment and final inspection, so a condition question that surfaces during quoting can be resolved before the order is released rather than after the first lot arrives.
Optional reader questions
Can a third-party heat treater age solution-treated stock without voiding the mill certification? The mill certification describes the material as the mill supplied it — solution treated, in this example. Aging by a qualified heat treater adds a process step; it does not rewrite the mill’s certificate. What changes is the evidence package: you now hold a mill cert for the solution-treated condition plus a heat-treat chart and, if you require it, property results from coupons aged with the parts. Write the order so the two records are linked by lot and heat number, and the certification chain stays intact.
How do AMS 5663 and ASTM B637 aged material differ in what the buyer receives? Both can deliver solution-treated-and-aged material with certified properties. They differ in the controlled document behind the cycle and in the aerospace flow-downs that come with the AMS document. If your drawing calls out one, order that one; do not treat the other as interchangeable on the strength of a cross-reference.
What if the mill cert cites a cross-referenced specification instead of the one on the drawing? Treat it as an open item. Ask the supplier to state, in writing, which specification and revision the delivered condition was produced to, and compare the solution treatment and aging cycle against your drawing’s callout. If the supplier cannot show that the delivered condition satisfies your specification, the material has not been demonstrated to conform, however sound it is.
Can hardness alone confirm the condition was applied? No. Hardness is one line in the acceptance table; B637 also requires tensile and stress-rupture results per lot. A hardness reading confirms that some aging happened, not that the specified cycle was run or that the other properties were met. Use the chart and the full test report, and treat hardness as a screening check rather than proof.